一般描述
Aluminum surfaces are not receptive to most plating processes due to their tendency to form oxides rapidly.Oxide formation inhibits uniform plating, resulting in inhomogeneous deposits, poor adhesion, or no deposition at all. By first applying Zincate Electroless Immersion Zinc Plating Solution to a properly prepared aluminum surface, it is possible subsequently deposit high quality electroless nickel films.
应用
Plating onto aluminum involves a multiple step process.
1.Non-etch clean the aluminum surface for up to 5 minutes with a detergent-based cleaner. Rinse thoroughly with cascading water.
2. De-smut the surface for 10-30 seconds using an acid mixture. RTM A for plastics is a suitable agent for smut removal. Rinse again thoroughly.
3. Mild etch for 5-10 seconds in a 25% solution of Aluminum Etch Type A. Rinse again thoroughly.
4. De-smut a second time and rinse as in step 2.
5. Apply the first Zincate layer. Immerse the part in the Zincate solution for 1-2 minutes at room temperature until a gray color develops. Rinse.
6. Remove the first Zincate layer using 50% nitric acid for 30-60 seconds or until the deposit turns white. Rinse.
7. Apply a second Zincate layer for 30-60 seconds. Rinse thoroughly before applying electroless nickel to the surface.
1.Non-etch clean the aluminum surface for up to 5 minutes with a detergent-based cleaner. Rinse thoroughly with cascading water.
2. De-smut the surface for 10-30 seconds using an acid mixture. RTM A for plastics is a suitable agent for smut removal. Rinse again thoroughly.
3. Mild etch for 5-10 seconds in a 25% solution of Aluminum Etch Type A. Rinse again thoroughly.
4. De-smut a second time and rinse as in step 2.
5. Apply the first Zincate layer. Immerse the part in the Zincate solution for 1-2 minutes at room temperature until a gray color develops. Rinse.
6. Remove the first Zincate layer using 50% nitric acid for 30-60 seconds or until the deposit turns white. Rinse.
7. Apply a second Zincate layer for 30-60 seconds. Rinse thoroughly before applying electroless nickel to the surface.
警示用语:
Danger
危险声明
危险分类
Aquatic Chronic 3 - Eye Dam. 1 - Met. Corr. 1 - Skin Corr. 1A
WGK
WGK 1
闪点(°F)
Not applicable
闪点(°C)
Not applicable
法规信息
新产品
我们的科学家团队拥有各种研究领域经验,包括生命科学、材料科学、化学合成、色谱、分析及许多其他领域.
联系技术服务部门